By Tony Tate · updated 2026-11-27 · First Layer 1.0.2
Foaming TPU (LW-TPU) prints at about 225 °C with a 45 °C bed and 30% part cooling. Usable range 200–250 °C nozzle, 25–60 °C bed. No enclosure needed.
LW-TPULightweight TPUVarioshoreFoaming flexible
Starting settings
starting points Every number here is drawn from
manufacturer data sheets across the material as a whole. None of it is a measurement of the
spool in your hand, and brand-to-brand variation inside one material is wider than most people
expect. Where a figure says "about", the app holds one typical value rather than a range. Treat
all of it as somewhere to begin, then measure — shrinkage and flow especially, because those two
are what throw dimensions off.
Nozzle
200–250 °C (start 225)
Bed
25–60 °C (start 45)
Part fan
0–50% (start 30%)
Wall speed
10–30 mm/s
Max volumetric flow
about 3 mm³/s
Shrinkage
about 0.6%
Glass transition
about -35 °C — flexible above it, so at room temperature it is rubbery rather than soft
Enclosure
Not needed
Nozzle size
0.4 mm or larger — 0.6 mm recommended
Nozzle material
Brass is fine
Drying
about 50 °C for 6 h
Speed
Slow, 10–30 mm/s. Expansion needs dwell time at temperature, so speed and density are linked here in a way they are not on any other material.
Bed surface
Clean smooth PEI at 45 °C.
Nozzle
0.6 mm suits it — the foamed extrusion is wider than the nozzle, and a bigger opening makes that easier to control.
What bites people
Temperature is a DENSITY setting on this material, not just a melt setting. Cooler prints denser and firmer, hotter prints lighter and spongier — a temperature tower here is reading softness, not surface quality.
Flow must come DOWN as temperature goes up, or the expansion over-extrudes. Roughly halve the flow at the hot end of the range; the exact figure is a per-spool measurement.
The extrusion is wider than the nozzle once it expands, which throws off any dimensional calibration done with a normal material.
Everything true of soft TPU is still true here — slow speeds, minimal retraction, direct drive preferred.
Safety
Nozzle above 200 °C.
Common questions
What temperature should I print Foaming TPU (LW-TPU) at?
Start at 225 °C nozzle and 45 °C bed, within a usable range of 200–250 °C and 25–60 °C. Run a temperature tower on your own spool rather than trusting any table: brand-to-brand variation inside one material is wider than most beginners expect.
Does Foaming TPU (LW-TPU) need an enclosure?
No. Foaming TPU (LW-TPU) prints fine on an open-frame machine.
What nozzle do I need for Foaming TPU (LW-TPU)?
0.4 mm or larger, with 0.6 mm recommended. A brass nozzle is fine.